Comparison of the strength and durability performance of normal- and
high-strength pozzolanic concretes at elevated temperatures
Chi-Sun Poon*, Salman Azhar, Mike Anson, Yuk-Lung Wong
Department of Civil and Structural Engineering, Research Center for Advanced Technology in Structural Engineering,
The Hong Kong Polytechnic University, Hung Hom, Hong Kong, China
Received 7 August 2000; accepted 18 June 2001
Abstract
The strength and durability performance of normal- and high-strength pozzolanic concretes incorporating silica fume, fly ash, and blast
furnace slag was compared at elevated temperatures up to 800C. The strength properties were determined using an unstressed residual
compressive strength test, while durability was investigated by rapid chloride diffusion test, mercury intrusion porosimetry (MIP), and crack
pattern observations. It was found that pozzolanic concretes containing fly ash and blast furnace slag give the best performance particularly at
temperatures below 600C as compared to the pure cement concretes. Explosive spalling occurred in most high-strength concretes (HSCs)
containing silica fume. A distributed network of fine cracks was observed in all fly ash and blast furnace slag concretes, but no spalling or
splitting occurred. The high-strength pozzolanic concretes showed a severe loss in permeability-related durability than the compressive
strength loss. Thirty percent replacement of cement by fly ash in HSC and 40% replacement of cement by blast furnace slag in normal-
strength concrete (NSC) was found to be optimal to retain maximum strength and durability after high temperatures. D 2001 Elsevier Science
Ltd. All rights reserved.
Keywords: High temperature; Pozzolan; Compressive strength; Permeability; Microstructure
1. Introduction
Pozzolanic concretes are used extensively throughout the
world; the oil, gas, nuclear, and power industries are among
the major users. The applications of such concretes are
increasing day by day due to their s