摘 要:研究捕收剂DLZ对黄铜矿和黄铁矿的浮选行为。浮选试验结果表明,DLZ对黄铜矿的捕收能力强,最大95.7%,而对黄铁矿的捕收能力弱,回收率小于10%。动电位分析发现与DLZ作用后,黄铜矿的动电位比黄铁DLZ对黄铜矿和黄铁矿的捕收有选择性。红外光谱分析表明DLZ在黄铜矿表面的吸附属
关键词:黄铜矿;黄铁矿;捕收剂;动电位
中图分类号:TD923.1 文献标识码:A 文章编号2010)02-0045-04
MECHANISM OF COLLECTOR-DLZ IN CHALCOPYRITE AND PYRITE FLOTATION
LI Jianhua, SUN Xiaojun
(Daye Nonferrous Metals Company, Huangshi Hubei 435005, China)
Abstract: The flotation behavior of DLZ was studied. Results of flotation experiments show that the collecting ability of DLZ to chalcopyrite is stronger than pyrite, the max recovery of chalcopyrite is 95.7%, the recovery of pyrite is less than 10%. Zeta potential analysis showed that the zeta potential of chalcopyrite decreased more than that of pyrite after interaction with DLZ, confirming that DLZ showed selectivity towards chalcopyrite and pyrite. FTIR results indicate that the adsorption of DLZ onto chalcopyrite surface is chemical absorption and onto the pyrite surface is physical adsorption.
Keywords: chalcopyrite; pyrite; collector; adsorption capacity; flotation
在硫化铜矿中,铜硫共生是一种常见的矿石类[1],但黄[2-5]。石灰用]。且被抑制的黄。DLZ对黄铜矿
L 试样、药剂及研究方法
1.1试样及药剂
黄铁矿取自广东云浮硫铁矿选厂,黄铜矿取自74+32μm粒46.2%、硫49.5%,纯度为93%,黄铜矿矿样含31.3%、铁29.5%、硫34.4%,酯度为90.5%。DLZ、氧化钙、盐酸和氢氧化钠均为分
1.2试验设备和研究方法
浮选试验用XFG型挂槽式浮选机,浮选槽容40mL;取纯矿物2.0g放进100mL烧杯中,加5min,澄清后倒去上清min后需调整剂,搅拌3min后加入起泡剂搅拌min,3min。泡沫产品和槽内产品分别烘干称重,
动电位试验。将矿样用玛瑙研钵研磨至5μm,每次称取50mg置于100mL中,加100m蒸馏水,HCl或NaOH调节pH值至合适值后,加入(或不)一定浓度的调整剂或捕收剂,搅拌5min,用Coulter Delsa 440sx分析仪进行电位测定。
红外光谱测定。将固体样品在玛瑙研钵中磨KBr粉料,继续研磨并混合均匀,然后将Nicolet FTIR-740型傅立叶
2 试验结果及讨论
2.1 DLZ的浮选性能
在铜硫分离时大多采用石灰抑制硫化铁矿物而NaOH、HCl和CaO调矿浆pH值时捕收剂对矿物可浮性的影响。定DLZ用量为2.610-6mol/L,起泡剂松醇油的用22mg/L,捕收剂DLZ的捕收性能与pH的关1所示。 由图l可知,用NaOH、HCl调矿浆pH值时,pH范围内(pH 2.7~12.05),黄铜矿的可浮95.7%;黄铁矿在整个pH范围内的可浮性都很差,最大回收率为24.1%,pH大于6.9以后,黄铁矿可浮性下降很快,回10%。用CaO调矿浆pH与NaOH相比,pH为7~1l时,CaO对黄铜矿的可浮性影响不pH为12时黄铜矿回收率下降较大,黄63.3%,CaO对黄铁矿的浮选有较强5%。
固pH为6.9,DLZ用量试验结果如图2所2可知,DLZ用量从2.610-6mol/L增加到15.6×1
显示全部